Protect the metal surface: Lessons in cooling water corrosion control
In November’s Field Notes Lunch & Learn, Chemical Processing editor-in-chief Traci Purdum welcomed back Brad Buecker, senior technical consultant with SAMCO Technologies, for part two of his cooling water series. Last month, he covered microbiological fouling. This time, he turned to corrosion: how it happens, how to control it and how treatment programs have changed.
Corrosion Fundamentals
Buecker described corrosion as an electrochemical process. In the classic example of steel in hydrochloric acid, iron dissolves at anodes while electrons travel to cathodic sites and reduce hydrogen ions. In cooling water, dissolved oxygen usually does the oxidizing, forming iron hydroxides that turn into rust. Those deposits can speed up corrosion beneath them. In buried piping he has seen, they choked off flow entirely.
The main factors are pH, conductivity, temperature and dissolved oxygen. Corrosion generally drops as pH rises, but iron is amphoteric, so very high pH also attacks it. Higher temperatures speed corrosion, but warmer water holds less oxygen.
Localized Attack is the Real Danger
Equipment life of 30 to 50 years is calculated from general corrosion rates. Localized mechanisms break that assumption. They include pitting, chloride attack on austenitic stainless steels, oxygen-ammonia attack on copper alloys, microbiologically influenced corrosion, manganese-induced corrosion, galvanic corrosion and stress corrosion cracking. These can cause failures within months while most of the metal is still sound. Buecker gave the example of steam surface condensers: A single pit through a tube wall lets cooling water into the high-purity condensate that returns to the boiler, and the damage can be severe.
From Chromate to Phosphate to Non-Phosphorus
Acid-chromate programs worked well and were easy to control, but they were banned because they release hexavalent chromium, a carcinogen. Their replacements, phosphate, phosphonate, polymer and zinc programs run at mildly alkaline pH, cut general corrosion but brought new problems, including calcium phosphate deposits and sensitivity to changes in water chemistry. Regulations then limited zinc, copper discharges and, starting in the 2010s, phosphorus as an aquatic nutrient.
The industry is now moving to non-phosphorus programs built on film-forming products, such as a polyhydroxy starch inhibitor, which bond to the metal and form a physical barrier. The approach follows the creed of cooling water expert Paul Puckorius: “Protect the metal surface.” Making it work requires:
- Thorough analysis of both makeup and cycled water.
- An estimate of the surface area to be protected.
- Vigilance against overfeed and breakdown by oxidizing biocides.
- Reliable monitoring.
For copper alloys, azoles such as benzotriazole, along with halogen-resistant versions, remain the standard.
Choose Materials Carefully
Buecker recalled reviewing specifications for combined-cycle plants in which designers specified 304L or 316L stainless steel condenser tubes out of habit. Just a few cycles of concentration would push chlorides past the recommended limits for those alloys. The pitting resistance equivalent number helps match an alloy to the chloride level. Superferritic grades such as Sea-Cure suit high-chloride and seawater service.
Monitoring
Corrosion coupons, usually left in place for 30 to 90 days, remain the industry standard, though mils-per-year guidelines can miss localized attack. Electrochemical probes provide real-time data.
Know Your Water
Buecker’s main advice was to know your water chemistry. He recommended the Cooling Technology Institute and the Association for Materials Protection and Performance, formerly NACE International, as resources. He shared an example from his career: During the 1988 drought, the lake feeding a once-through cooling system concentrated fourfold. Calcium carbonate scaled a stainless steel condenser, while units with admiralty brass tubes stayed clean. As he and Purdum agreed, “It can never happen” are dangerous words.